init commit
This commit is contained in:
@@ -0,0 +1,443 @@
|
||||
# Hacker Fab PMOS -- Al gate / Al2O3 gate dielectric -- Silvaco Victory flow
|
||||
# Layout: Pmos.gds (cell "Pmos", um) -- put it in the DeckBuild working dir.
|
||||
#
|
||||
# WHY THE PROCESS ORDER CHANGED vs. the poly-gate deck
|
||||
# Aluminum melts at 660 C, so the gate cannot exist during the 1100 C boron
|
||||
# drive-in. The flow is therefore "diffusion first, gate last":
|
||||
# S/D boron SOD (patterned) -> drive-in -> strip -> ALD Al2O3 -> Al gate
|
||||
# -> 700B SOG -> contacts (SOG + Al2O3) -> Al contacts / pads
|
||||
# The gate is no longer self-aligned: it overlaps the S/D only because the
|
||||
# boron spreads laterally under the gate edge during the drive-in. GateOv
|
||||
# (S/D mask offset) and SDTime set that overlap.
|
||||
# Victory Process cannot anneal once Al2O3 is in the structure (material
|
||||
# table: Al2O3 diffusion "-"), which this order also respects.
|
||||
#
|
||||
# Masks (GDS layer -> Victory Process mask name "L#<layer>.<datatype>")
|
||||
# Pattern 1 S/D boron SOD diff 65/20 AND NOT poly 66/20 (2 etches)
|
||||
# Pattern 2 Al gate poly 66/20 (Al kept inside polygons)
|
||||
# Pattern 3 Contacts li1 67/20 REVERSE (SOG + Al2O3 opened inside)
|
||||
# Pattern 4 Contact metal met1 68/20 (Al kept inside polygons)
|
||||
# Not used: nwell (wafer is n-type), psdm/nsdm, mcon (0.28 um, below litho).
|
||||
#
|
||||
# Gate dielectric: ALD Al2O3, material "Al2O3" (Victory Process material ID 229);
|
||||
# its permittivity is set to the ALD value (KAlOx) in the device modules.
|
||||
# If Victory Device rejects "Al2O3", replace every material=Al2O3 with
|
||||
# material=sapphire (the Al2O3 name both simulators are documented to know).
|
||||
#
|
||||
# Domain: transistor symmetric about x = 25 (gate centre) and y = 0.
|
||||
# 2D: x 25..38.5 cut at y = 0, mirrored in x.
|
||||
# 3D: x 25..38.5, y 0..7.5 after removing the uniform stripe y = 4..10
|
||||
# (LAYOUT.REMOVE.Y), mirrored in x; y = 0 is a symmetry plane and
|
||||
# currents are normalized by the simulated half-width Wn = 6.5 um.
|
||||
#
|
||||
# Device simulation is split into three modules (transfer / output / gate
|
||||
# leakage). Each ends with a "go internal" DeckBuild extract block, so the same
|
||||
# extraction runs in DeckBuild and in Victory DoE (VDoE manual sec. 12.4).
|
||||
# In Victory DoE the three device modules can run in parallel.
|
||||
#
|
||||
# Conventions: cleans/resist/expose/develop/strip = comments; wet etches =
|
||||
# ETCH WET in 2D, ETCH DRY in 3D (memory); spin-on films = deposited oxide;
|
||||
# furnace steps = inert anneals. NEVER put a # comment on a line ending in "\".
|
||||
|
||||
SET name="HF_PMOS_Al"
|
||||
|
||||
SET dim = "2D" # "2D" = cut through y = 0 (fast) / "3D"
|
||||
SET save_vis = 0 # 1 = Victory Visual .str after key steps (2D only)
|
||||
|
||||
# -P N = threads. Session has ~4-5 cores and ~2.1 GB: 2D -P 4, 3D -P 1.
|
||||
GO victoryprocess simflags="-P 4"
|
||||
|
||||
## ---------------------------------- ##
|
||||
## ------- Layout-derived geometry ---- ##
|
||||
## -----------------------------------##
|
||||
SET Xg = 25.0 # Gate centre (poly 22.917..27.083)
|
||||
SET Lgate = 4.1667 # Drawn gate length
|
||||
SET W = 25.0 # Gate width (diff y -12.5..12.5)
|
||||
SET Xge = $Xg+$Lgate/2 # Gate edge (27.083)
|
||||
SET Xdiff = 37.5 # Diff edge in x
|
||||
SET Ydiff = 12.5 # Diff edge in y
|
||||
SET Xd = 33.333 # Drain contact centre (li1 31.667..35.0)
|
||||
SET Xs = 16.667 # Source contact centre after mirroring
|
||||
SET Xmax = 38.5 # Domain edge in x
|
||||
SET Ymax = 13.5 # Domain edge in y (2D cut / unsqueezed)
|
||||
# 3D "squeeze": the channel is uniform in y between the contacts/metal
|
||||
# (|y| <= 3.5) and the diff edge (12.5). LAYOUT.REMOVE.Y cuts y = 4..10 out of
|
||||
# the layout (manual: INIT LAYOUT.REMOVE.Y) and closes the gap, so the 3D
|
||||
# domain keeps every 3D feature (contacts, metal, diff edge, gate ends) with
|
||||
# ~45% less area. Simulated half-width = 12.5 - 6.0 = 6.5 um.
|
||||
SET Ysq = 6.0 # width of the removed stripe (um)
|
||||
|
||||
## ---------------------------------- ##
|
||||
## ------- DOE process knobs ---------- ##
|
||||
## -----------------------------------##
|
||||
SET RhoSub = 10 # n-type wafer resistivity (ohm-cm)
|
||||
SET Tsod = 0.25 # Boron SOD thickness (um) -- calibrate
|
||||
SET Csod_B = 5.0e20 # Boron SOD effective concentration -- calibrate to Rs
|
||||
SET SDTime = 30 # S/D drive-in time (min)
|
||||
SET SDTemp = 1100 # S/D drive-in temperature (C)
|
||||
SET GateOv = 0.0 # S/D mask pull-back from the drawn gate edge (um per
|
||||
# side). >0: S/D starts further from the gate (less
|
||||
# overlap); <0: S/D drawn under the gate.
|
||||
SET Tal2o3 = 0.020 # ALD Al2O3 gate dielectric thickness (um)
|
||||
|
||||
## ---------------------------------- ##
|
||||
## ------- Other film parameters ------ ##
|
||||
## -----------------------------------##
|
||||
SET TalG = 0.50 # Gate Al thickness (um), thermal evaporation
|
||||
SET GateBias = 0.0 # Gate mask bias (um per edge, DELTACD)
|
||||
SET Tsog = 0.30 # 700B SOG thickness (um) -- calibrate
|
||||
SET Tal = 0.50 # Contact Al thickness (um)
|
||||
SET AlBias = 0.0 # Contact-metal mask bias (met1 encloses li1 by 1.83 um)
|
||||
|
||||
## ---------------------------------- ##
|
||||
## ------- Wet-etch model ------------ ##
|
||||
## -----------------------------------##
|
||||
# 2D: ETCH WET (isotropic). 3D: ETCH DRY (WET over 3D topography runs out of
|
||||
# memory). The gate Al wet etch undercuts by ~its thickness; in 3D that undercut
|
||||
# is reproduced by shrinking the gate mask (GateUC) so 2D and 3D gates match.
|
||||
if cond=($dim="2D")
|
||||
SET etchm = "wet"
|
||||
SET Tclr = 0.02
|
||||
SET TclrAl = 0.05
|
||||
SET GateUC = 0.0
|
||||
if.end
|
||||
if cond=($dim="3D")
|
||||
SET etchm = "dry"
|
||||
SET Tclr = 0.02
|
||||
SET TclrAl = 0.10+$TalG+$Tsog
|
||||
SET GateUC = $TalG+0.05
|
||||
if.end
|
||||
|
||||
## ---------------------------------- ##
|
||||
## -------- Step 0: Substrate -------- ##
|
||||
## -----------------------------------##
|
||||
# n-type wafer; native oxide removed by the BOE dip before the SOD spin.
|
||||
# Grid: finest cell = resolution/16 (meshdepth=3) must be <= ~1/1.5 of the
|
||||
# thinnest layer (20 nm Al2O3; manual sec. 2.10.3).
|
||||
# 2D 0.16 -> 10 nm. 3D "0.32, 0.40, 0.21" -> 20 / 25 / 13 nm (low accuracy,
|
||||
# fits ~2.1 GB). Gas height 3 um holds the stack (1.32 um) plus the barrier
|
||||
# layer masked ETCH WET deposits.
|
||||
if cond=($dim="3D")
|
||||
INIT material=silicon orientation=100 dopants=phosphorus resistivity=$RhoSub \
|
||||
depth=3.0 gasHeight=3.0 LAYOUT="Pmos.gds" CELL="Pmos" \
|
||||
LAYOUT.REMOVE.Y="4.0, 10.0" \
|
||||
FROM="25.0,0.0" TO="38.5,7.5" FLOW.DIM=3D \
|
||||
resolution="0.32, 0.40, 0.21" meshdepth=3
|
||||
if.end
|
||||
if cond=($dim="2D")
|
||||
INIT material=silicon orientation=100 dopants=phosphorus resistivity=$RhoSub \
|
||||
depth=3.0 gasHeight=3.0 LAYOUT="Pmos.gds" CELL="Pmos" \
|
||||
FROM=$Xg TO=$Xmax AT=0 FLOW.DIM=2D_XZ \
|
||||
resolution=0.16 meshdepth=3
|
||||
if.end
|
||||
|
||||
# Doping (volume-data) mesh
|
||||
if cond=($dim="2D")
|
||||
SET sxg = 0.05
|
||||
SET sxd = 0.10
|
||||
SET szs = 0.01
|
||||
SET szj = 0.03
|
||||
if.end
|
||||
if cond=($dim="3D")
|
||||
SET sxg = 0.20
|
||||
SET sxd = 0.30
|
||||
SET szs = 0.03
|
||||
SET szj = 0.08
|
||||
if.end
|
||||
|
||||
LINE x location=$Xg spacing=0.5
|
||||
LINE x location=$Xge spacing=$sxg
|
||||
LINE x location=$Xge+1.5 spacing=0.4
|
||||
LINE x location=$Xdiff spacing=$sxd
|
||||
LINE x location=$Xmax spacing=0.5
|
||||
if cond=($dim="3D")
|
||||
LINE y location=0 spacing=1.5
|
||||
LINE y location=$Ydiff-$Ysq spacing=0.4
|
||||
LINE y location=$Ymax-$Ysq spacing=0.5
|
||||
if.end
|
||||
LINE z location=-3.0 spacing=0.50
|
||||
LINE z location=-1.5 spacing=0.20
|
||||
LINE z location=-0.55 spacing=0.10
|
||||
LINE z location=0.0 spacing=$szs
|
||||
LINE z location=0.3 spacing=$szj
|
||||
LINE z location=1.5 spacing=0.15
|
||||
LINE z location=3.0 spacing=0.50
|
||||
|
||||
## ---------------------------------- ##
|
||||
## ---- S/D boron SOD (pattern 1) ---- ##
|
||||
## -----------------------------------##
|
||||
# Acetone + IPA clean; BOE dip (native oxide) (no-op)
|
||||
# Spin-on dopant (boron, e.g. Filmtronics B153/B155), 4000 rpm, 20 s
|
||||
DEPOSIT conformal material=oxide thickness=$Tsod dopants=boron dopingvalues=$Csod_B
|
||||
|
||||
# HMDS / spin AZ P4210 / bake / stepper litho -- Pattern 1: S/D = diff NOT gate
|
||||
# Develop, then BOE 6:1 10 s removes the SOD outside the S/D windows:
|
||||
# (a) outside diff
|
||||
ETCH $etchm material=oxide thickness=$Tsod+$Tclr MASK="L#65.20"
|
||||
# (b) over the gate area (poly polygon grown by GateOv per side)
|
||||
ETCH $etchm material=oxide thickness=$Tsod+$Tclr MASK="L#66.20" REVERSE DELTACD=$GateOv
|
||||
# Wet strip resist (no-op)
|
||||
|
||||
# S/D drive-in, inert (tube furnace)
|
||||
# AUTOREF=false: keep the grid fixed during the anneal (inert, no moving
|
||||
# surfaces; adaptive refinement only costs memory).
|
||||
DIFFUSE time=$SDTime min temperature=$SDTemp AUTOREF=false
|
||||
|
||||
# BOE 6:1, 10 min -- strip SOD glass
|
||||
ETCH $etchm material=oxide thickness=$Tsod+$Tclr
|
||||
|
||||
SAVE name=$'name'_VP_SD
|
||||
if cond=($save_vis=1)
|
||||
if cond=($dim="2D")
|
||||
SAVE name=$'name'_VP_SD conformalstr
|
||||
if.end
|
||||
if.end
|
||||
|
||||
## ---------------------------------- ##
|
||||
## ---- Gate stack (pattern 2) ------- ##
|
||||
## -----------------------------------##
|
||||
# ALD Al2O3 gate dielectric (no anneals are possible after this point)
|
||||
DEPOSIT conformal material=Al2O3 thickness=$Tal2o3
|
||||
|
||||
# Thermal evaporation Al (gate)
|
||||
DEPOSIT conformal material=aluminum thickness=$TalG
|
||||
|
||||
# HMDS / spin / bake / stepper litho -- Pattern 2: gate (poly 66/20) / develop
|
||||
# Type A Al etchant, 40 C -- keep Al inside the gate polygons; stops on Al2O3.
|
||||
ETCH $etchm material=aluminum thickness=$TalG+0.05 MASK="L#66.20" DELTACD=$GateBias-$GateUC
|
||||
# Wet strip resist (no-op)
|
||||
|
||||
SAVE name=$'name'_VP_Gate
|
||||
if cond=($save_vis=1)
|
||||
if cond=($dim="2D")
|
||||
SAVE name=$'name'_VP_Gate conformalstr
|
||||
if.end
|
||||
if.end
|
||||
|
||||
## ---------------------------------- ##
|
||||
## ---- ILD + contacts (pattern 3) --- ##
|
||||
## -----------------------------------##
|
||||
# Spin-coat 700B SOG, 4000 rpm, 20 s (modeled conformal).
|
||||
# The 200 C / 10 min bake is omitted: thermally negligible, and Victory Process
|
||||
# cannot run DIFFUSE with Al2O3 in the structure.
|
||||
DEPOSIT conformal material=oxide thickness=$Tsog
|
||||
|
||||
# HMDS / spin / bake / stepper litho -- Pattern 3: contacts (li1 67/20) / develop
|
||||
# BOE 6:1 -- open SOG, then Al2O3, inside the contact polygons
|
||||
ETCH $etchm material=oxide thickness=$Tsog+$Tclr MASK="L#67.20" REVERSE
|
||||
ETCH $etchm material=Al2O3 thickness=$Tal2o3+0.005 MASK="L#67.20" REVERSE
|
||||
# Wet strip resist (no-op)
|
||||
|
||||
SAVE name=$'name'_VP_Contact
|
||||
|
||||
## ---------------------------------- ##
|
||||
## ---- Contact metal (pattern 4) ---- ##
|
||||
## -----------------------------------##
|
||||
# Thermal evaporation Al
|
||||
DEPOSIT conformal material=aluminum thickness=$Tal
|
||||
|
||||
# Clean / spin / bake / stepper litho -- Pattern 4: metal (met1 68/20) / develop
|
||||
# Type A Al etchant -- keep Al inside met1 (gate Al is protected by the SOG)
|
||||
ETCH $etchm material=aluminum thickness=$Tal+$TclrAl MASK="L#68.20" DELTACD=$AlBias
|
||||
# Wet strip resist (no-op)
|
||||
|
||||
SAVE name=$'name'_VP_Metal
|
||||
|
||||
## ---------------------------------- ##
|
||||
## ------ Mirror & electrodes -------- ##
|
||||
## -----------------------------------##
|
||||
MIRROR mirror="-x"
|
||||
if cond=($dim="3D")
|
||||
ELECTRODES name=gate x=$Xg+0.5 y=0.5 z=-($Tal2o3+$TalG/2)
|
||||
ELECTRODES name=source x=$Xs y=0.5 z=-0.1
|
||||
ELECTRODES name=drain x=$Xd y=0.5 z=-0.1
|
||||
ELECTRODES substrate
|
||||
if.end
|
||||
if cond=($dim="2D")
|
||||
ELECTRODE name=gate x=$Xg+0.5 z=-($Tal2o3+$TalG/2)
|
||||
ELECTRODE name=source x=$Xs z=-0.1
|
||||
ELECTRODE name=drain x=$Xd z=-0.1
|
||||
ELECTRODE name=substrate substrate
|
||||
if.end
|
||||
|
||||
if cond=($dim="2D")
|
||||
SAVE name=$'name'_VP_sv conformalstr
|
||||
if.end
|
||||
if cond=($dim="3D")
|
||||
SAVE name=$'name'_VP_sv
|
||||
if.end
|
||||
|
||||
GO victorymesh simflags="-P 4"
|
||||
####### STRUCTURE REMESHING #######
|
||||
LOAD in=$'name'_VP_sv
|
||||
# Junction is ~1-1.5 um deep; 2.5 um keeps it with margin and trims the mesh.
|
||||
CROP axis = "z" offset = "2.5"
|
||||
REMESH conformal
|
||||
SAVE out=$'name'_VM_con.str
|
||||
|
||||
####### DEVICE SIMULATION #######
|
||||
# Three modules: (A) transfer, (B) output, (C) gate leakage. All biases are
|
||||
# negative (PMOS). Coarse bias steps on purpose (speed).
|
||||
|
||||
## ===== (A) Transfer: Id-Vg at Vd = -Vdlin and Vd = -Vdd ===== ##
|
||||
GO victorydevice simflag="-P 4"
|
||||
|
||||
SET Vdd = 5.0
|
||||
SET Vgmax = 2.0 # sweeps start at +2 V (off) and go to -Vdd
|
||||
SET Vdlin = 0.1
|
||||
SET Vgleak = 10.0 # 10 V / 20 nm = 5 MV/cm (Al2O3 breaks down ~5-8 MV/cm)
|
||||
SET WF = 4.1 # Al gate work function (eV)
|
||||
SET KAlOx = 9.0 # ALD Al2O3 relative permittivity
|
||||
SET Qf = -1.0e12 # Al2O3/Si fixed charge (cm^-2); ALD Al2O3 is negative
|
||||
SET Tau = 1.0e-6 # SRH lifetimes (s); realistic for a clean wafer
|
||||
if cond=($dim="2D")
|
||||
SET Wn = 1.0 # 2D: width=1 -> currents in A/um
|
||||
if.end
|
||||
if cond=($dim="3D")
|
||||
SET Wn = $W/2-$Ysq # 3D: simulated half-width (y = 0 symmetry plane, squeezed)
|
||||
if.end
|
||||
|
||||
if cond=($dim="2D")
|
||||
MESH infile=$'name'_VM_con.str width=1
|
||||
if.end
|
||||
if cond=($dim="3D")
|
||||
MESH infile=$'name'_VM_con.str
|
||||
if.end
|
||||
CONTACT name=gate workfunction=$WF
|
||||
MATERIAL material=Al2O3 permittivity=$KAlOx
|
||||
INTERFACE qf=$Qf
|
||||
MATERIAL material=silicon taun0=$Tau taup0=$Tau
|
||||
MODELS fermi srh cvt fldmob print
|
||||
METHOD newton maxtrap=10
|
||||
|
||||
SOLVE init
|
||||
SOLVE previous
|
||||
SOLVE vstep=0.5 vfinal=$Vgmax name=gate
|
||||
SOLVE vdrain=-0.01
|
||||
SOLVE vstep=-0.05 vfinal=-$Vdlin name=drain
|
||||
SAVE outfile=tA_lowD
|
||||
SOLVE vstep=-$Vdd/5 vfinal=-$Vdd name=drain
|
||||
SAVE outfile=tA_highD
|
||||
|
||||
LOAD infile=tA_lowD
|
||||
LOG outfile=$'name'_VD_IdVg_lin.log
|
||||
SOLVE vstep=-0.25 vfinal=-$Vdd name=gate
|
||||
LOG off
|
||||
|
||||
LOAD infile=tA_highD
|
||||
LOG outfile=$'name'_VD_IdVg_sat.log
|
||||
SOLVE vstep=-0.25 vfinal=-$Vdd name=gate
|
||||
LOG off
|
||||
|
||||
go internal
|
||||
# Signed PMOS values (Vt negative). Currents normalized to A/um via Wn.
|
||||
SET Io = 1e-7
|
||||
extract init infile="HF_PMOS_Al_VD_IdVg_lin.log"
|
||||
extract name="Vtgm_V" (xintercept(minslope(curve(v."gate",abs(i."drain")))) - ave(v."drain")/2.0)
|
||||
extract name="Vtlin_V" x.val from curve(v."gate",abs(i."drain")) where y.val=$Io*$Wn/$Lgate
|
||||
extract name="Idlin_A" y.val from curve(v."gate",abs(i."drain")) where x.val=-$Vdd
|
||||
extract name="Idlin_uA_um" $"Idlin_A"*1e6/$Wn
|
||||
extract init infile="HF_PMOS_Al_VD_IdVg_sat.log"
|
||||
extract name="Vtsat_V" x.val from curve(v."gate",abs(i."drain")) where y.val=$Io*$Wn/$Lgate
|
||||
extract name="Idsat_A" y.val from curve(v."gate",abs(i."drain")) where x.val=-$Vdd
|
||||
extract name="Idsat_uA_um" $"Idsat_A"*1e6/$Wn
|
||||
extract name="Ioff_A" y.val from curve(v."gate",abs(i."drain")) where x.val=0.0
|
||||
extract name="Ioff_pA_um" $"Ioff_A"*1e12/$Wn
|
||||
extract name="SSsat_mV_dec" -1000.0/slope(minslope(curve(v."gate",log10(abs(i."drain")))))
|
||||
extract name="DIBL_mV" ($"Vtsat_V" - $"Vtlin_V")*1000.0
|
||||
|
||||
## ===== (B) Output: Id-Vd, Vg = -1 .. -5 V ===== ##
|
||||
GO victorydevice simflag="-P 4"
|
||||
if cond=($dim="2D")
|
||||
MESH infile=$'name'_VM_con.str width=1
|
||||
if.end
|
||||
if cond=($dim="3D")
|
||||
MESH infile=$'name'_VM_con.str
|
||||
if.end
|
||||
CONTACT name=gate workfunction=$WF
|
||||
MATERIAL material=Al2O3 permittivity=$KAlOx
|
||||
INTERFACE qf=$Qf
|
||||
MATERIAL material=silicon taun0=$Tau taup0=$Tau
|
||||
MODELS fermi srh cvt fldmob print
|
||||
METHOD newton maxtrap=10
|
||||
|
||||
SOLVE init
|
||||
SOLVE previous
|
||||
SAVE outfile=tB_zero
|
||||
|
||||
LOAD infile=tB_zero
|
||||
SOLVE vstep=-0.5 vfinal=-1.0 name=gate
|
||||
LOG outfile=$'name'_VD_IdVd_Vg1.log
|
||||
SOLVE vdrain=0.0
|
||||
SOLVE vstep=-0.5 vfinal=-$Vdd name=drain
|
||||
LOG off
|
||||
|
||||
LOAD infile=tB_zero
|
||||
SOLVE vstep=-0.5 vfinal=-2.0 name=gate
|
||||
LOG outfile=$'name'_VD_IdVd_Vg2.log
|
||||
SOLVE vdrain=0.0
|
||||
SOLVE vstep=-0.5 vfinal=-$Vdd name=drain
|
||||
LOG off
|
||||
|
||||
LOAD infile=tB_zero
|
||||
SOLVE vstep=-0.5 vfinal=-3.0 name=gate
|
||||
LOG outfile=$'name'_VD_IdVd_Vg3.log
|
||||
SOLVE vdrain=0.0
|
||||
SOLVE vstep=-0.5 vfinal=-$Vdd name=drain
|
||||
LOG off
|
||||
|
||||
LOAD infile=tB_zero
|
||||
SOLVE vstep=-0.5 vfinal=-4.0 name=gate
|
||||
LOG outfile=$'name'_VD_IdVd_Vg4.log
|
||||
SOLVE vdrain=0.0
|
||||
SOLVE vstep=-0.5 vfinal=-$Vdd name=drain
|
||||
LOG off
|
||||
|
||||
LOAD infile=tB_zero
|
||||
SOLVE vstep=-0.5 vfinal=-5.0 name=gate
|
||||
LOG outfile=$'name'_VD_IdVd_Vg5.log
|
||||
SOLVE vdrain=0.0
|
||||
SOLVE vstep=-0.5 vfinal=-$Vdd name=drain
|
||||
LOG off
|
||||
|
||||
go internal
|
||||
extract init infile="HF_PMOS_Al_VD_IdVd_Vg5.log"
|
||||
extract name="IdVd5_A" max(abs(i."drain"))
|
||||
extract name="IdVd5_uA_um" $"IdVd5_A"*1e6/$Wn
|
||||
|
||||
## ===== (C) Gate leakage: Ig-Vg, Vd = Vs = Vsub = 0 ===== ##
|
||||
# Fowler-Nordheim tunneling only in this module (it slows every solve).
|
||||
# Note: the built-in FN coefficients are for SiO2; for Al2O3 (lower barrier)
|
||||
# the absolute Ig is indicative only -- compare trends between splits.
|
||||
GO victorydevice simflag="-P 4"
|
||||
if cond=($dim="2D")
|
||||
MESH infile=$'name'_VM_con.str width=1
|
||||
if.end
|
||||
if cond=($dim="3D")
|
||||
MESH infile=$'name'_VM_con.str
|
||||
if.end
|
||||
CONTACT name=gate workfunction=$WF
|
||||
MATERIAL material=Al2O3 permittivity=$KAlOx
|
||||
INTERFACE qf=$Qf
|
||||
MATERIAL material=silicon taun0=$Tau taup0=$Tau
|
||||
MODELS fermi srh cvt fldmob fn.cur print
|
||||
METHOD newton maxtrap=10
|
||||
|
||||
SOLVE init
|
||||
SOLVE previous
|
||||
LOG outfile=$'name'_VD_IgVg.log
|
||||
SOLVE vstep=-1.0 vfinal=-$Vgleak name=gate
|
||||
LOG off
|
||||
|
||||
go internal
|
||||
extract init infile="HF_PMOS_Al_VD_IgVg.log"
|
||||
extract name="Ig_Vdd_A" y.val from curve(v."gate",abs(i."gate")) where x.val=-$Vdd
|
||||
extract name="Ig_Vgleak_A" y.val from curve(v."gate",abs(i."gate")) where x.val=-$Vgleak
|
||||
|
||||
#### PLOTS (DeckBuild only; one window each) ####
|
||||
victoryvisual $'name'_VM_con.str
|
||||
victoryvisual $'name'_VD_IdVg_lin.log+$'name'_VD_IdVg_sat.log
|
||||
victoryvisual $'name'_VD_IdVd_Vg1.log+$'name'_VD_IdVd_Vg2.log+$'name'_VD_IdVd_Vg3.log+$'name'_VD_IdVd_Vg4.log+$'name'_VD_IdVd_Vg5.log
|
||||
victoryvisual $'name'_VD_IgVg.log
|
||||
|
||||
quit
|
||||
Reference in New Issue